Breadcrumb
Process Flow: Deposit and Anneal a Thin Film
Find an Instrument › Fabricate › Deposit and anneal a thin film
Outline. MATFab staff are still checking these steps.
The usual sequence of steps at MATFab, with the tool for each step.
- Solvent clean the substrate (acetone, IPA, dry) · bench work (ask staff)
- O2 plasma clean (optional) · Harrick plasma cleaner
- Deposit the film · IntlVac Nanochrome II sputter. Metals can also be evaporated (NexDep e-beam or Edwards thermal evaporator).
- Measure the thickness as deposited · Woollam ellipsometer. For transparent films on a flat substrate. For opaque films, measure a step at a masked edge with the Veeco Wyko optical profiler.
- Anneal · MTI RTP annealer. Ask staff which gases are connected. For long, low-temperature bakes use the VWR vacuum oven.
- Measure again after the anneal · Woollam ellipsometer
Each step links to the tool in the Instrument Selection Guide. Ask MATFab staff before your first run.