Find an Instrument › Fabricate › Plasma-bond PDMS to glass

Outline. MATFab staff are still checking these steps.

The usual sequence of steps at MATFab, with the tool for each step.

  1. Mix the PDMS and degas it · VWR vacuum oven. A vacuum desiccator also works.
  2. Pour onto the mold and cure · bench work (ask staff). An oven or a hotplate; ask staff which one is allowed for PDMS.
  3. Peel the PDMS, cut it to size and punch the inlets · bench work (ask staff)
  4. Clean the glass (solvent, dry) · bench work (ask staff)
  5. Treat the PDMS and the glass in an O2 plasma · Harrick plasma cleaner. The activated surfaces lose their bonding ability quickly. Next step within: a few minutes.
  6. Press the two surfaces together · bench work (ask staff)
  7. Bake to strengthen the bond · bench work (ask staff). An oven or a hotplate.

Each step links to the tool in the Instrument Selection Guide. Ask MATFab staff before your first run.